Specifications of EN 10083-3 Alloy Steel Plate
Standard: EN 10083-3, which outlines the technical delivery conditions for alloy steels intended for quenching and tempering.
Available Grades: 41Cr4, 25CrMo4, 34CrMo4, and 42CrMo4.
Delivery Condition: Plates can be delivered in a hot-rolled, annealed, or normalized and tempered state.
Dimensions:
Thickness: 5 mm to 100 mm
Width: 1000 mm, 1200 mm, 1500 mm, 1800 mm
Length: 3000 mm, 6000 mm, 12000 mm
EN 10083-3 Alloy Steel Plate Chemical Composition
Steel designation |
Chemical composition % by massa,b |
||||||||||
Name |
Number |
C |
Si max. |
Mn |
P max. |
S |
Cr |
Mo |
Ni |
V |
B |
Steels without boron c |
|||||||||||
41Cr4 |
1.7035 |
0,38 to 0,45 |
0,40 |
0,60 to 0,90 |
0,025 |
max. 0,035 |
0,90 to 1,20 |
- |
- |
- |
- |
25CrMo4 |
1.7218 |
0,22 to 0,29 |
0,40 |
0,60 to 0,90 |
0,025 |
max. 0,035 |
0,90 to 1,20 |
0,15 to 0,30 |
- |
- |
- |
34CrMo4 |
1.7220 |
0,30 to 0,37 |
0,40 |
0,60 to 0,90 |
0,025 |
max. 0,035 |
0,90 to 1,20 |
0,15 to 0,30 |
- |
- |
- |
42CrMo4 |
1.7225 |
0,38 to 0,45 |
0,40 |
0,60 to 0,90 |
0,025 |
max. 0,035 |
0,90 to 1,20 |
0,15 to 0,30 |
- |
- |
- |
a Elements not quoted in this table shall not be intentionally added to the steel without the agreement of the purchaser, other than for the purpose of finishing the heat and for boron to have its effect on the hardenability. All reasonable precautions shall be taken to prevent the addition of such elements from scrap or other material used in the manufacture which affect the hardenability, mechanical properties and applicability. |
|||||||||||
b Where requirements are made on hardenability (see Tables 5 and 6) or on the mechanical properties in the quenched and tempered condition (see Table 8), slight deviations from the limits for the cast analysis are permissible, except for the elements carbon, phosphorus and sulfur; the deviations shall not exceed the specifications of Table 4. |
|||||||||||
c Steels with improved machinability as a result of the addition of higher sulphur contents up to around 0,10% S (including resulphurized steels with controlled inclusion content (e.g. Ca-treatment)) may be supplied on request. In this case the upper limit for the manganese content may be increased by 0,15 %. |
EN 10083-3 Alloy Steel Plate Mechanical Properties at Room Temperature in The Quenched and Tempered Condition (+QT)
Steel designation |
Mechanical properties for the ruling section (see EN 10083-1:2006, Annex A) with a diameter (d) or for flat products thickness (t) of |
|||||||||||||||||||||||||
d = 16 mm |
16 mm < d = 40 mm 8 mm < t = 20 mm |
40 mm < d = 100 mm 20 mm < t = 60 mm |
100 mm < d = 160 mm 60 mm < t = 100 mm |
160 mm < d = 250 mm 100 mm < t = 160 mm |
||||||||||||||||||||||
t = 8 mm |
||||||||||||||||||||||||||
Name |
Number |
Re |
Rm |
A |
Z |
KV |
Re |
Rm |
A |
Z |
KV |
Re |
Rm |
A |
Z |
KV |
Re |
Rm |
A |
Z |
KV |
Re |
Rm |
A |
Z |
KV |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
min. |
|
|
|
|
|
|
|
MPa |
% |
% |
J |
MPa |
% |
% |
J |
MPa |
% |
% |
J |
MPa |
% |
% |
J |
MPa |
% |
% |
J |
|
|
|
|
|
|
|
41Cr4 |
1.7035 |
800 |
1000 to |
11 |
30 |
- |
660 |
900 to |
12 |
35 |
35 |
560 |
800 to |
14 |
40 |
35 |
- |
- |
- |
- |
- |
- |
- |
- |
- |
- |
25CrMo4 |
1.7218 |
700 |
900 to |
12 |
50 |
- |
600 |
800 to |
14 |
55 |
50 |
450 |
700 to |
15 |
60 |
50 |
400 |
650 to |
16 |
60 |
45 |
- |
- |
- |
- |
- |
34CrMo4 |
1.7220 |
800 |
1000 to |
11 |
45 |
- |
650 |
900 to |
12 |
50 |
40 |
550 |
800 to |
14 |
55 |
45 |
500 |
750 to |
15 |
55 |
45 |
450 |
700 to |
15 |
60 |
45 |
42CrMo4 |
1.7225 |
900 |
1100 to |
10 |
40 |
- |
750 |
1000 to |
11 |
45 |
35 |
650 |
900 to |
12 |
50 |
35 |
550 |
800 to |
13 |
50 |
35 |
500 |
750 to |
14 |
55 |
35 |
EN 10083-3 Alloy Steel Plate Heat Treatment Sheets
Steel designation |
Quenching |
Quenching agent |
Tempering |
End quench test |
|
Name |
Number |
°C |
°C |
°C |
|
41Cr4 |
1.7035 |
820 to 860 |
Oil or water |
540 to 680 |
850 ± 5 |
25CrMo4 |
1.7218 |
840 to 900 |
Water or oil |
540 to 680 |
850 ± 5 |
34CrMo4 |
1.7220 |
830 to 890 |
Oil or water |
540 to 680 |
850 ± 5 |
42CrMo4 |
1.7225 |
820 to 880 |
Oil or water |
540 to 680 |
850 ± 5 |